← Technologies, Filler Materials and Equipment

Production of Spherical Powders for 3D Printing by Ultrasonic Atomization and by Plasma-Arc Atomization of Bar Stock of Boron-Microalloyed AISI 420 Stainless Steel Produced by Electroslag Remelting

Vadym Petruk1 0000-0003-0742-0131, Ganna Polishko1 0000-0001-7543-280X, Volodymyr Korzhyk1 0000-0001-9106-8593, Yurii Bogomol2 0000-0001-6633-0078, Dmytro Strohonov1, Oleksii Tereshchenko1 0009-0003-4021-0758, Yevhenii Illiashenko1 0000-0001-9876-0320, Alla Tunik1 0000-0001-6801-6461

  1. 1E.O. Paton Electric Welding Institute of the National Academy of Sciences of Ukraine
  2. 2E.O. Paton Electric Welding Institute of the National Academy of Sciences of Ukraine, Igor Sikorsky Kyiv Polytechnic Institute (National Technical University of Ukraine)

Oral Online

The paper considers two methods of producing fine spherical powders from the metal of electroslag remelting (ESR) ingots — ultrasonic atomization on a sonotrode, and plasma-arc atomization of rod stock made from the ingots using a transferred arc of reverse polarity. Experimental ingots 50 mm in diameter and about 150 mm long, made of AISI 420 steel additionally alloyed with boron and niobium, were produced by ESR on a laboratory USh-114 unit in a stationary water-cooled mould.

In the first method, spherical powders were obtained by ultrasonic atomization using the AMAZEMET rePOWDER and reMELTER system (Poland). Rods prepared by longitudinal cutting of the ESR ingots were melted by electric arc melting, and droplets of the melt flowed down into the crucible-waveguide. Atomization was carried out by dispersing the melt film on the waveguide in a flowing argon atmosphere. The frequency of the ultrasonic system was 40 kHz, and the melting current was 270 A.

In the second method, the powder was produced by plasma-arc atomization of rod stock in an argon atmosphere on a unit developed at the E.O. Paton Electric Welding Institute. The rod was clamped in a linear-feed mechanism with a low-speed rotary drive (50 rpm) and connected to the negative pole of the power source. A transferred plasma arc at a current of 200 A was formed between the rod (cathode) and the internal anode electrode of the plasmatron; the argon flow rate was 100 L/min. The molten metal at the rod end face was dispersed by a high-velocity plasma jet, with subsequent break-up, spheroidization and solidification of the droplets.

Ultrasonic atomization yielded batches of spherical powder with a particle size of 35–70 µm and a mean size of 47 µm. The powder produced by plasma-arc atomization of bars with a transferred arc showed a broad particle size distribution in the range of 45 to 400 µm. According to scanning electron microscopy, all batches are dominated by particles of regular spherical shape with a smooth surface and a fine-cellular dendritic relief; satellites were practically absent. Isolated agglomerates of the fine fraction are present in insignificant amounts.

Local X-ray spectral microanalysis of individual particles showed that the alloying complex of the parent metal is retained: chromium 11.83–12.43 %, molybdenum 9.57–10.99 %, nickel 0.18–0.66 %, niobium 1.26–1.30 %. The boron content was monitored by classical (wet) chemical analysis: according to preliminary data, up to 0.086 wt. % in the parent metal.

Thus, ultrasonic atomization of rod stock made of AISI 420 steel produced by electroslag remelting ensures the formation of predominantly spherical powder particles while preserving the main complex of alloying elements of the parent material. The dominant fraction of the resulting powder is 35–70 µm with a mean particle size of about 47 µm. After classification, the fraction with particle sizes up to 60 µm may, in terms of its granulometric characteristics, be regarded as potentially suitable for further trials in laser powder bed fusion (LPBF/SLM), in particular for the formation of gradient bulk structures. Fractions with particle sizes up to 100 µm may be studied as a powder material for direct laser deposition (DLD). Plasma-arc atomization of rod stock makes it possible to obtain spherical powders over a wider size range — approximately 45–400 µm. Individual fractions of these powders may, in terms of their granulometric characteristics, be promising for plasma powder surfacing, additive manufacturing by directed energy deposition, and — after appropriate classification — for electron-beam additive manufacturing. Coarser fractions may be of interest for powder metallurgy processes, in particular hot isostatic pressing and the production of porous preforms with subsequent infiltration.