Diffusion welding of magnesium alloy to aluminium alloy using a titanium interlayer
Lidiia PETRUSHYNETS 0000-0001-7946-3056, Iurii FALCHENKO
0000-0002-3028-2964, Viktor FEDORCHUK
0000-0002-9929-3231
- Paton Electric Welding Institute of the National Academy of Sciences of Ukraine
Oral Online
Because of their low density, magnesium alloys are promising materials for mechanical engineering and other weight-sensitive industries, but their low strength and high corrosion limit their use. Alloying and aluminium coatings improve properties. Joining magnesium and aluminum alloys combines their benefits, but welding is difficult because of their different properties and brittle Mg-Al intermetallics that weaken joints. Diffusion welding (DW) with optimized temperatures and interlayers controls or eliminates these phases, improving joint strength and durability.
Sheets of MA2-1 (Mg-Al-Zn system) magnesium alloy and AMts (Al-Mn system) aluminium alloy with thicknesses of 1.4 mm and 0.5 mm, respectively, were investigated. A 50-μm-thick VT1-0 commercially pure titanium foil was utilized as an interlayer.
The Mg/Al bimetallic joints were fabricated via a two-step diffusion welding process. In the first step, the aluminium alloy was joined to the titanium foil under the following conditions: T = 560 °C, P = 10 MPa, t = 30 min. The resulting Al/Ti bimetal was subsequently welded to the magnesium alloy at 440 °C and 10 MPa for 30 min. The welding experiments were conducted using specialized fixtures enabling a gradient pressure distribution via stainless steel mesh interlayers. Following the welding process, the specimens were post-weld annealed in air at 250 °C for 60 min.
The experiments produced defect-free joints. Metallographic examination of the welded Mg/Ti/Al specimens revealed that the joint zone exhibits a nearly planar cross-sectional shape, with only minor waviness observed at the Mg/Ti interface. Diffusion processes proceeded slowly; the TiAl₃ intermetallic phase with a thickness of up to 1 μm began to form at the Al/Ti interface. On the titanium alloy side, the Mg/Ti interface consists of an α-Ti phase containing magnesium, with its concentration remaining below the solubility limit of Mg in α-Ti.
Annealing at 250 °C promotes diffusion processes at the joint. Visually, this is manifested by increased waviness both along the Mg/Ti joint line and at the Al/Ti interface. Mutual diffusion of alloy components leads to the formation of a two-phase band up to 5 μm thick at the Mg/Ti interface, consisting of α-Ti and an Mg-enriched phase, with an Mg content of 54.34 at.%. The width of the TiAl₃ intermetallic phase along the Al/Ti interface does not change; however, the aluminium content in this layer decreases to nearly 50 at.%. The decrease in Al concentration compared with TiAl₃ may be associated with mutual diffusion of Al and Ti, as well as averaging of the EDS signal within the thin gradient layer.
Based on the obtained results, it can be concluded that post-welding annealing at T = 250 °C for t = 60 min does not lead to the formation of new intermetallic compounds of the Al-Ti system; however, it promotes intensification of diffusion processes, resulting in the formation of wavy joint zones with lower gradients of chemical element concentrations.