Grain-boundary strengthening of Magnesium Alloys during FSW
Maksym Khokhlov 0000-0002-8180-3459, Valery Kostin
0000-0002-2677-4667, Julia Khokhlova
0000-0002-2145-973X
- Е. О. Раton Electric Welding Institute
Oral in Person
In previous studies, the formation of the stress-strain state during friction stir welding (FSW) was considered as a thermodynamic macro-process and modeled for three linear welding speeds (8, 16 and 25 m/h) at a constant rotational speed of the FSW tool. The theoretical residual stresses and strains along and transverse to the weld were determined under thermoelastic deformation conditions. Experimentally measured Young’s modulus (E) and microhardness (H) were determined in the welded joint according to ISO 14577-1:2015 and were used in the residual stress-strain model. The next stage of the study expands the understanding of the mechanism governing the formation of the stress-strain state during FSW by visualizing the features of the atomic structure of Mg alloy and investigating the Hall-Petch effect – yield strength and hardness increase with decreasing grain size in the nugget zone of the Mg alloy FSW joint.
Thermodynamic processes at FSW temperatures above 600°C form a typical narrow interface on the retreating side (RS), approximately 100 μm wide, between the stir zone (SZ) and the thermomechanically affected zone (TMAZ). Local microcrystalline texture flows develop in the stir zone (SZ) and the core zone (CZ). The base material (BM) has a typical rolled microstructure with elongated 100-200 μm grains, which is preserved in the heat-affected zone (HAZ), formed at ~380-450°C. The non-uniform plastic flow of the metal alters the microstructure of the TMAZ and it shows the lowest hardness, making it the critical zone for fracture under tensile loading.
The mechanism by which a volume of the metal flow is captured was visualized by thermomechanically asymmetric map of viscoplastic flow. The simulation was done using the Coupled Eulerian-Lagrangian (CEL) method in Abaqus/Explicit. The constitutive behavior of the material was described by the Johnson-Cook model, while the contact interaction by the modified Coulomb-Tresca law. The resulting map exhibits typical angular segments of laminar flow, displaced toward the retreating side (RS) by the lateral surface of the pin.
Five different slip modes can be activated in the HCP crystal lattice of the α-Mg matrix during FSW: prismatic (3 slip systems), basal (3 slip systems), pyramidal (6 slip systems), first-order pyramidal (12 slip systems), second-order pyramidal (6 slip systems). This allows extreme levels of deformation without the loss of structural integrity. The denser β-Mg₁₇Al₁₂ is hard and brittle intermetallic phase with a complex cubic crystal lattice that strengthens Mg-Al alloys. Its Young’s modulus increases with increased pressure, indicating higher resistance to volumetric and shear deformations and overall stiffness. The phase remains undeformed until the brittle-to-ductile transition is reached at ~300°C.
Experimentally, in SZ obtained at the lowest linear welding speed, a threefold increase in the elastic modulus and microhardness was observed in CZ, representing a classical Hall-Petch effect. An increase in hardness indicates an increase in yield strength. It was established that when the grain size decreases below 20 nm (SEM), an inverse Hall-Petch effect occurs, whereby the hardness decreases to a level of BM. Thus, a linear welding speed of 16 m/h is a limiting effective FSW speed, at which Hall-Petch effect was not observed and an amorphized texture developed in CZ and SZ had properties comparable to those of BM with a reduced level of the stress-strain state.