← Technologies, Filler Materials and Equipment

THE EFFECT OF MICROSTRUCTURAL DISPERSITY IN WELDED JOINTS ON THEIR SUSCEPTIBILITY TO PLASTIC DEFORMATION DURING LASER WELDING OF STAINLESS STEEL

Yurii Yurchenko 0000-0001-9253-009X, Oleksandr Siora 0009-0005-8542-1633, Valentyna Bondarieva 0000-0002-4745-0995, Mykola Sokolovskyi 0000-0003-3243-5060, Artemii Bernatskyi 0000-0002-8050-5580

  1. E. O. Paton Electric Welding Institute of the National Academy of Sciences of Ukraine

Oral Online

Welding is one of the key manufacturing processes in modern industry, enabling the production and assembly of critical thin-walled structures. Stainless steels are widely used in the chemical, oil and gas, energy, food processing, and automotive industries, as well as in the manufacture of heat exchangers, pressure vessels, and piping equipment, due to their combination of high strength, resistance to aggressive environments, and ability to maintain their performance properties at elevated temperatures. Laser welding is a promising method for producing such joints; due to its high energy concentration, narrow heat-affected zone, and minimal deformation, it ensures high-quality joints in thin-walled structural elements. Obtaining welded joints with high mechanical properties is a prerequisite for ensuring the reliability and durability of such structures.

AISI 304 stainless steel with a thickness of 1.5 mm was selected as the material for butt welds. Laser welding was performed at a constant energy density of 60 J/mm within a power range of P = 1.5…2.5…3.5 kW; welding speeds of V = 1.5…2.5…3.5 m/min; and a laser beam defocusing value of ΔF = 0 mm.

The mechanical properties of the joints were evaluated based on the results of static tensile testing and three-point bending. Failure of all specimens during tensile testing occurred in the base metal zone. As the laser power increases, the maximum values of the yield strength increase slightly: the increase compared to 1.5 kW is approximately 1.4% at 2.5 kW and 2.7% at 3.5 kW. For the tensile strength, this trend is more pronounced – the increase reaches approximately 1% and 4%, respectively. At the same time, as welding power and speed increase, the variation in the values of yield strength and tensile strength also increases.

Three-point bending tests (at angles of 90° and 180°, with the weld face and root facing outward) revealed no fractures or cracks, confirming the absence of defects such as porosity, undercut, and lack of fusion, in accordance with DSTU EN ISO 13919-1:2015.

To establish a relationship between welding parameters and microstructural behavior under tensile loads, cross-sections of the welded joints were prepared after tensile testing, and their geometric parameters were measured. It was found that an increase in laser power from 1.5 to 3.5 kW is accompanied by a decrease in both the initial and final geometric parameters of the weld. At the same time, a clear inverse relationship was observed between laser power and the weld metal’s susceptibility to transverse plastic deformation: the relative increase in weld area after tensile testing monotonically decreases from 71.62% at 1.5 kW to 35.59% at 3.5 kW. This is explained by the fact that at the maximum power of 3.5 kW, a more dispersed microstructure of the weld is formed. The long grain boundaries in such a structure, in accordance with Hall–Petch’s law, increase the material’s resistance to plastic deformation and effectively suppress transverse plastic deformation during mechanical loading.

Thus, laser welding is a promising method for producing butt joints in thin-walled corrosion-resistant steels, since the high crystallization rates of the weld pool contribute to the refinement of the weld microstructure, which positively affects its mechanical properties.