The effect of the induction crucible-free zone melting process on the structure and properties of the intermetallic alloy of the Ti-Al-Nb-Zr-Co-LaB6 alloying system.
Tsyhichko Stanislav1 0000-0000-0000-0000, Piskun Nataliia1
0000-0001-1459-2321, Voron Mikhail2
0000-0000-0000-0000, Statkevich Ihor1
0000-0001-9403-2123, Motrrii Vitalii1
0000-0001-5820-1161
- 1E.O. Paton Electric Welding Institute (PWI)
- 2Physico-Technological Institute of Metals and Alloys of the National Academy of Sciences of Ukraine
Oral Online
Modern aviation and space engineering is developing under conditions of strict requirements for increasing fuel efficiency, reducing emissions and increasing engine thrust. Traditional nickel superalloys remain the main materials for the most critical high-temperature parts of gas turbine engines, however, their high density significantly increases the mass of the rotor. Therefore, intermetallic alloys based on γ-TiAl, due to their low density, high specific strength, creep resistance and oxidation resistance, are considered as an alternative for individual components of the hot section, primarily low-pressure turbine blades.
In recent years, a new class of TiAl-based alloys, the so-called TNM alloys, has been developed and is being considered. The high content of β-stabilizing elements Nb and Mo leads to the preservation of some amount of the primary β(Ti) phase with a disordered bcc structure or its ordered low-temperature modification B2. β(Ti) plays a positive role in improving the machinability and application of TNM alloys.
The Institute of Electric Welding has proposed a new intermetallic alloy of the alloying system 52Ti-30Al-11Nb-4Co-2Zr-1LaB6. The developed alloy has significant advantages over the new generation TNM-type alloys, since Zr and Nb also stabilize the β-phase, but they are lighter than Mo, and the created alloy has a lower density, which is a strong argument for the aerospace industry. Co improves strength, wear resistance, heat resistance and corrosion resistance, LaB6 reduces cracking and porosity during welding, binds harmful impurities and stabilizes the structure at high temperatures. The density of the resulting alloy is 4.11 g/cm3, which is almost 1.7 times less than that of TNM alloys (6.9 g/cm3).
Structural studies and mechanical tests of the primary ingot showed that it had an uneven coarse microstructure, inhomogeneous distribution of elements across the ingot field, as well as micropores and microcracks. All these shortcomings determined its low mechanical properties at room and high temperatures.
Typically, before using a cast intermetallic alloy to eliminate these defects, it must be subjected to gas static isothermal pressing (GIP), heat treatment for many hours, or hot rolling.
One of the ways to improve the structure and increase the mechanical characteristics of an intermetallic is directional crystallization. For directional crystallization, we have proposed the crucible-free zone melting (CZM) method. In CZM, the existence of a stable molten zone is ensured by surface tension forces. The advantages of CZM are that without the use of GIP treatment, the ingots obtained do not have microdefects - breaks, microcracks, etc., and there is no porosity, since shrinkage occurs directionally at the crystallization front, and not in the volume of the ingot. CZM allows you to control the structure of the resulting material. By changing the parameters of the melting process, you can obtain the required structure of the ingot. In addition, CZM conditions ensure the purity of the process - there is no interaction with the crucible material.
The work has studied the starting material of the developed intermetallic alloy and after BZP treatment. According to the results of the research, the distribution of alloy elements and structural components along the length of the ingot was determined. The influence of BZP on structural transformations in the ingot and ensuring the uniformity of the distribution of elemen